As welded | |||||
淇濊(h霉)姘i珨 | 灞堟湇寮�(qi谩ng)搴� | 寤朵几鐜� | 鎶楁媺寮�(qi谩ng)搴� | Stress Relieved Temperature | Stress Relieved Testing Time |
AWS 80Ar/20CO2(M21) | 715 MPa | 17 % | 805 MPa | - | - |
EN 80Ar/20CO2(M21) | 730 MPa | 19 % | 800 MPa | - | - |
Stress relieved | |||||
淇濊(h霉)姘i珨 | 灞堟湇寮�(qi谩ng)搴� | 寤朵几鐜� | 鎶楁媺寮�(qi谩ng)搴� | Stress Relieved Temperature | Stress Relieved Testing Time |
EN 80Ar/20CO2(M21) | 690 MPa | 20 % | 750 MPa | 620 掳C | 15 hr |
As welded | ||||
淇濊(h霉)姘i珨 | 娌栨搳鍊� | 娓�(c猫)瑭︽韩搴� | Stress Relieved Testing Temp | Stress Relieved Testing Time |
AWS 80Ar/20CO2(M21) | 80 J | -30 掳C | - | - |
AWS 80Ar/20CO2(M21) | 60 J | -40 掳C | - | - |
EN 80Ar/20CO2 (M21) | 100 J | 20 掳C | - | - |
EN 80Ar/20CO2 (M21) | 73 J | -40 掳C | - | - |
Stress relieved | ||||
淇濊(h霉)姘i珨 | 娌栨搳鍊� | 娓�(c猫)瑭︽韩搴� | Stress Relieved Testing Temp | Stress Relieved Testing Time |
EN 80Ar/20CO2 (M21) | 130 J | 20 掳C | 620 掳C | 15 hr |
EN 80Ar/20CO2 (M21) | 60 J | -20 掳C | 620 掳C | 15 hr |
EN 80Ar/20CO2 (M21) | 60 J | -30 掳C | 620 掳C | 15 hr |
Mn | Mo | C | Si | Ni | Cr |
1.54 % | 0.24 % | 0.089 % | 0.53 % | 1.23 % | 0.26 % |
瀹夊煿 | 鐔旀暦鐜� | 闆诲 V | 鐩村緫 | 閫佺挡閫熷害 |
80-280 A | 1-5,4 kg/h | 18-28 V | 0.8 mm | 2,7-14,7 m/min |
80-280 A | 1-5,4 kg/h | 18-28 V | 0.9 mm | 2,7-14,7 m/min |
80-280 A | 1-5,4 kg/h | 18-28 V | 1.0 mm | 2,7-14,7 m/min |
120-350 A | 1,5-6,6 kg/h | 20-33 V | 1.2 mm | 2,7-12,4 m/min |
225-480 A | 3,3-0 kg/h | 26-38 V | 1.6 mm | 3,1-8,1 m/min |
瑾�(r猫n)璀�: | ER 110S-G (M21), ABS, EN 13479, CE, 42.039.33, DB, IV Y69MS (M21), DNV-GL, 11837, VdT眉V, 1.2MM, NAKS/HAKC |
鍒嗛: | G 69 4 M Mn3Ni1CrMo, EN ISO 16834-A, G Mn3Ni1CrMo, EN ISO 16834-A, Wire Electrode, ER110S-G, SFA/AWS A5.28, Wire Electrode |
瑾�(r猫n)璀夊潎鍩轰簬宸ュ粻鐨勬墍鍦ㄥ湴銆傚闇€鏇村淇℃伅锛岃珛(q菒ng)鑱�(li谩n)绯讳紛钖�銆�
鍚堥噾椤炲瀷: | Low alloyed (1.4 % Ni, 0.3 % Cr, 0.3 % Mo) |